If you have a kiln and have a lot of scrap glass, then this is a great way to use that scrap glass to create really lovely creative fused glass pendants and more. The shapes available are heart, circle, square and tear drop.
Use with transparent and opaque glass to make your own unique glass pieces. These molds are for pot melts, yet small enough to fit in smaller sized kilns! Use MR97 Boron Nitride spray on all molds.
Fill the Mini Scrap Master with the glass scraps with the weights of glass listed below, then place the Scrap Master on top of the Cast-A-Cab mold in your kiln.
LF124 Hearts = 1.1 oz - 1.3 oz/heart,
LF125 Circles = 1.2 oz - 1.4 oz/circle,
LF126 Squares = 1.3 oz - 1.5 oz/square
LF127 Tears = 1.1 oz - 1.3 oz /tear
LF125 Circles = 1.2 oz - 1.4 oz/circle,
LF126 Squares = 1.3 oz - 1.5 oz/square
LF127 Tears = 1.1 oz - 1.3 oz /tear
Use this Scrap Master suggested kiln schedule:
450 degrees per hr to 1660 degrees, hold 60 minutes
9999 degrees per hr to 1500 degrees, hold 30 minutes
9999 degrees per hr to 960 degrees, hold 90 minutes
100 degrees per hr to 825 degrees, hold 10 minutes
100 degrees per hr to 550 degrees, hold 5 minutes